Abstract:
|
Prevulcanized natural rubber latex was prepared
by the heating of the latex compound at 55°C for
different periods of time (2, 4, 6, 8, and 10 h). The changes in
the colloidal stability and physical properties were evaluated
during the course of prevulcanization. The prevulcanized
latex compounds were stored for 300 days, and the
properties were monitored at different storage intervals (0,
20, 40, 60, 120, 180, 240, and 300 days). During prevulcanization,
the mechanical stability time increased, and the viscosity
remained almost constant. The tensile strength increased
during storage for a period of 20 days. The degree of
crosslinking, modulus, elongation at break, and chloroform
number were varied with the time of storage. |